BP-based. Ballmill the non-metal chemicals together for 1-2 hours. Add the metal; Ti, FeTi, Iron, etc. Add 10% (of the non-metal comp, 2.5 ounces per 25 ounce mill batch) denatured alcohol to dampen thoroughly. As an alternative, the resin and hexamine may be dissolved in the alcohol, versus milling it with the dry mix. Pump at 1200-1900 psi on the comp. Cure overnight in a hot, 140160 degree, drying chamber. The hexamine will cause the resin to cross-link and bind the comet thoroughly. Prime, if necessary, with BP-paste and BP granules. The comp presses to a density of 1 ounce per 1 cubic inch. One 29.5 ounce batch (25 ounces of non-metal ingredients milled in a 5-quart mill barrel) will make a 3.5″ diameter x 3.5″ tall comet which burns from both ends for 6 seconds. One 29.5 ounce batch will make two 3.5″ diameter x 1.75″ tall rising comet tails for 12″ shells, which burn for 6 seconds from the one exposed end. The comp, made into comets, therefore, burns at 1 second per 1/4″.